What is the heat treatment process for electronic scale molds

Source:www.jnsgmm.com      Release date: 2025-09-08
The heat treatment process of electronic scale molds needs to be combined with their core requirements - high dimensional stability (to avoid deformation affecting weighing accuracy), moderate hardness (to balance processability and wear resistance), low internal stress (to prevent long-term use cracking), and also need to be adapted to commonly used mold materials (such as pre hardened plastic mo
       The heat treatment process of electronic scale molds needs to be combined with their core requirements - high dimensional stability (to avoid deformation affecting weighing accuracy), moderate hardness (to balance processability and wear resistance), low internal stress (to prevent long-term use cracking), and also need to be adapted to commonly used mold materials (such as pre hardened plastic mold steel 718H, ordinary plastic mold steel P20, or 45 # steel for metal structural component molds). The following is a typical process flow and key link description:
1、 Core premise: Material selection and pre-processing
      Different materials correspond to different heat treatment schemes. Electronic scale molds are mainly "plastic molds" (such as shell and tray molds), with a few being metal structural component molds. Pre treatment is the foundation for ensuring stable subsequent processes
1. Material matching:
      Mainstream choice: 718H (pre hardened plastic mold steel) - has reached 28-32HRC at the factory, does not require overall quenching, only local aging strengthening is needed;
      Economic choice: P20/45 # steel - requires "quenching and tempering+surface hardening" to achieve performance, suitable for low precision, small batch molds.
2. Pre treatment (stress relief annealing):
      Purpose: To eliminate internal stress caused by forging/rough machining of mold blanks and avoid deformation during subsequent heat treatment;
      Process: Heat to 600-650 ℃, hold for 2-4 hours (depending on the mold size), slowly cool in the furnace to below 200 ℃, and remove from the furnace;
      Key: For complex cavities (such as anti slip patterns on electronic scale trays), an additional stress relief annealing is required after rough machining and before precision machining.
2、 Mainstream Process: Typical Heat Treatment Process by Material
1. Pre hardened steel (718H): local strengthening+stabilization treatment (most commonly used)
      The 718H has been pre hardened to 28-32HRC before leaving the factory, and does not require overall quenching (to avoid deformation of the mold cavity). Only the parts that are prone to wear (such as parting surfaces and gates) need to be strengthened and the processing stress eliminated
Step 1: Stress relief after rough machining
      Heat to 550-580 ℃, hold for 3 hours, then cool in the furnace to 300 ℃ and air cool out of the furnace (temperature below the critical point of Ac1 to avoid phase transition) to eliminate the stress generated by rough milling.
Step 2: Local surface hardening (optional)
      If the mold parting surface and gate require higher wear resistance (to prevent long-term opening and closing wear), low-temperature nitriding should be used:
      Temperature: 450-500 ℃, keep warm for 15-20 hours;
      Effect: A 5-15 μ m nitride layer is formed on the surface, with a hardness of 60-70HRC, and the core still maintains 28-32HRC (balancing toughness and preventing cracking).
Step 3: Stable aging after precision machining
      Precision machining of molds (after the completion of key dimensions such as cavities and positioning holes), heating to 500-520 ℃, holding for 4-6 hours, and slow cooling with the furnace;
      Purpose: To further stabilize the organization (reduce dimensional drift during subsequent use), while releasing precision machining stress, ensuring that the cavity size error of the electronic scale mold is ≤ 0.02mm after long-term use (meeting the assembly accuracy of weighing components).
2. Ordinary mold steel (P20/45 # steel): quenched and tempered+surface hardened (economical type)
      P20/45 # steel is not pre hardened and needs to be quenched and tempered to obtain basic strength, followed by surface strengthening to improve wear resistance. It is suitable for electronic scale shell molds with low precision requirements:
Step 1: Quenching and tempering treatment (overall performance improvement)
      Quenching: Heat to 830-860 ℃ (upper limit for P20, lower limit for 45 # steel), hold for 1-2 hours (depending on thickness), and cool with oil to room temperature;
      High temperature tempering: Heat to 580-620 ℃, hold for 2-3 hours, and air cool;
Effect: The hardness reaches 22-26HRC, the microstructure is composed of martensite, and it combines strength and machinability, laying the foundation for subsequent precision machining.
Step 2: Surface quenching (local wear-resistant strengthening)
      Induction heating surface quenching is used for vulnerable parts such as parting surfaces and gates
      Temperature: 900-950 ℃, rapid heating (to avoid phase transition in the core), water spray cooling;
      Effect: The surface hardness reaches 50-55HRC, the depth of the hardened layer is 0.5-1mm, and the core still maintains 22-26HRC (anti brittle fracture).
Step 3: Low temperature stress relief tempering
      After surface quenching, heat to 180-200 ℃, hold for 2 hours, and air cool;
Purpose: To eliminate internal stress caused by surface quenching and prevent cracking during mold use.
3、 Key control steps: avoiding deformation and ensuring accuracy
      The electronic scale mold has high requirements for dimensional accuracy (such as the coaxiality between the mold cavity and the installation position of the weighing sensor), and it is necessary to focus on controlling three aspects:
Heating rate:
      When heating large molds (such as electronic scale platform panel molds), the rate should be ≤ 100 ℃/hour to avoid thermal stress deformation caused by excessive temperature difference;
Cooling method:
       Pre hardened steel (718H): slow cooling or air cooling throughout the furnace, water cooling is prohibited (to prevent cracking);
       Ordinary steel quenching and tempering: oil cooling (45 # steel) or water-soluble quenching agent cooling (P20) after quenching to avoid deformation caused by too fast cooling rate;
Time stability:
       After precision machining, 1-2 aging treatments (500-520 ℃) must be carried out, and key dimensions must be measured after each insulation until the dimensions are stable (change ≤ 0.005mm).
4、 Process validation: performance testing
      After heat treatment, two core tests are required to ensure that the usage requirements are met:
Hardness testing:
      Core hardness: 28-32HRC required for 718H, 22-26HRC required for P20/45 # steel;
Surface hardening layer: After nitriding/quenching, it needs to reach 50-70HRC (depending on the location requirements);
Dimensional inspection:
      Use a coordinate measuring instrument to detect the size of the mold cavity and the position of the positioning hole, with an error of ≤ 0.02mm (to avoid affecting the assembly and weighing accuracy of the electronic scale).
日韩福利视频网,日韩av二区在线播放,欧美日韩国产高清,婷婷精品在线
国产一区2区| 国产精品第十页| 国产一区不卡| 久久丁香四色| 久久av导航| 欧美精品99| 久久免费影院| bbw在线视频| 中文字幕高清在线播放| 欧美xxxx中国| 黑人精品一区| 国产一区国产二区国产三区| 91亚洲成人| 日韩毛片在线| 91精品91| 男女男精品网站| 日本中文字幕一区二区| 日本不卡视频一二三区| 日韩精品欧美大片| 国产精品一级在线观看| 久久精品国产久精国产| 91亚洲人成网污www| 欧美天堂视频| 不卡在线一区二区| 日韩一区精品视频| 日本麻豆一区二区三区视频| 日韩福利视频导航| 久久av偷拍| 蜜桃视频在线网站| 午夜精品婷婷| 日韩区一区二| 精品久久亚洲| 国产一区观看| 亚洲精品第一| 精品淫伦v久久水蜜桃| 91av亚洲| 在线成人直播| 日韩欧美另类中文字幕| 日本欧美大码aⅴ在线播放| 国产精品久久久久久久久免费高清| 久久三级中文| 欧美成人基地 | 六月丁香综合在线视频| 国产一区二区三区四区| 久久精品中文| 一区二区精彩视频| 麻豆91小视频| 国产一区二区三区自拍| 日韩精品亚洲一区二区三区免费| 另类欧美日韩国产在线| 日韩和的一区二在线| 蜜桃久久av一区| 国内自拍视频一区二区三区| 久久一区二区三区电影| 日韩欧美高清一区二区三区| 精品国产午夜肉伦伦影院| 1024精品一区二区三区| 日本午夜精品| 天堂√8在线中文| 亚洲aⅴ网站| 在线观看精品| 国产日产精品_国产精品毛片| 日韩在线免费| 国产麻豆一区| 亚洲一区二区三区免费在线观看| 国产精品久久久久久久久久久久久久久 | 亚洲啊v在线| 一二三区精品| 中文字幕色婷婷在线视频| 老司机久久99久久精品播放免费| 国产乱人伦丫前精品视频| 伊人精品一区| 国产精品三级| 美女国产一区| 国产精品二区不卡| 日韩欧美激情| 欧美亚洲在线日韩| 国产精品亚洲综合久久| 国产免费成人| 成人在线免费观看网站| 天堂成人国产精品一区| 成人影视亚洲图片在线| 亚洲精品三级| 欧美va天堂| 三上亚洲一区二区| 国产精品中文字幕亚洲欧美| 国产一区成人| 肉色欧美久久久久久久免费看 | 欧美日韩中文字幕一区二区三区 | 亚洲精品综合| 国产99久久| 精品一区二区三区中文字幕视频| 在线精品亚洲| 欧美天堂亚洲电影院在线观看| 久久精品国产亚洲aⅴ| 日韩国产在线观看一区| 国产精品丝袜xxxxxxx| 久久免费高清| 精品视频免费| 国产精品一区亚洲| 一区二区三区网站| 国产一区二区高清| 99精品综合| 国产成人77亚洲精品www| 国产精品视频一区视频二区| 美国三级日本三级久久99| av亚洲在线观看| 久久精品国内一区二区三区水蜜桃| 卡一卡二国产精品| 欧美精品97| 久久wwww| 欧美国产极品| 麻豆精品在线播放| 国产探花一区| 国产日产高清欧美一区二区三区| 日产欧产美韩系列久久99| 日韩影院精彩在线| 日韩在线观看一区二区| 国产精品人人爽人人做我的可爱| 久久黄色影院| 久久影院午夜精品| 成人日韩av| 欧美国产美女| 97国产精品| 日韩久久一区二区三区| 日韩国产网站| 九九在线精品| 中日韩男男gay无套| 羞羞答答国产精品www一本| 激情91久久| 国产精品毛片在线看| 男人操女人的视频在线观看欧美| 香蕉久久久久久久av网站| 丝袜脚交一区二区| 美国三级日本三级久久99| 丝瓜av网站精品一区二区 | 99国产精品私拍| 天堂成人国产精品一区| 亚洲综合激情在线| 日韩高清欧美激情| 国产精品对白久久久久粗| 国产在线视频欧美一区| 丁香六月综合| 欧美日韩中文一区二区| 99视频精品| 亚洲精品高潮| 国产精品hd| 欧美男人天堂| 久久久影院免费| 亚洲综合日本| 欧美日韩在线精品一区二区三区激情综合 | 亚洲午夜在线| 亚洲中午字幕| 欧美日韩视频免费看| 欧美精品二区| 久久精品卡一| 亚洲+小说+欧美+激情+另类| 国产精品一线天粉嫩av| 亚洲精品福利电影| 欧美成人午夜| 日本综合精品一区| 欧美激情日韩| 婷婷综合六月| 丝袜美腿一区二区三区| 国产精品伦一区二区| 在线观看精品| 综合色一区二区| 久久不见久久见中文字幕免费| 欧美日韩视频网站| 丝袜国产日韩另类美女| 国产精品视频一区二区三区| 国产精品久久久久av电视剧| 亚洲欧美日韩国产一区二区| 91免费精品国偷自产在线在线| 精品美女在线视频| 亚洲精品一区二区妖精| 日本午夜免费一区二区| 国产成人精品一区二区三区视频| japanese国产精品| 国产日产高清欧美一区二区三区| 国产综合色区在线观看| 亚洲毛片视频| 精品国产网站| 亚洲视频电影在线| 日韩成人综合| 日韩成人精品一区二区三区| 日本综合字幕| 国产午夜精品一区在线观看| 亚洲五月婷婷| 国产乱码精品一区二区亚洲| 香蕉精品视频在线观看| 国产精品久久久网站| 不卡视频在线| 国产一区二区亚洲| 日本亚州欧洲精品不卡| 肉色欧美久久久久久久免费看| 色狠狠一区二区三区| 成人午夜国产| 麻豆精品新av中文字幕| 中文字幕亚洲影视|